參數 | GMW15919 | Ford BI 107-05 | LP-463PB-64-01 |
流量 | 目標值2.7L/Min | 目標值2.7L/Min | 目標值2.7L/Min |
樣品測試位置溫度 | 98-100℃ | 98-100℃ | 98-100℃ |
油箱壓力 | 約50psi | 約50psi | 約50psi |
動態壓力 | 目標值37.9Kpa(5.5Psi) | 目標值37.9Kpa(5.5Psi) | 目標值37.9Kpa(5.5Psi) |
噴嘴和樣品距離 | 50-75mm | 50-75mm | 50-75mm |
噴嘴和樣品角度 | 45° | 45° | 45° |
噴嘴直徑 | 12.25 to 12.75mm | 12.25 to 12.75mm | 12.25 to 12.75mm |
噴嘴長度 | >100mm | >100mm | >100mm |
THERMAL SHOCK PROCEDURE FOR ORGANIC COATING ADHESION TEST
涂層系統附著力測試的熱沖擊程序
1.0 GENERAL
Test procedure is designed to evaluate the adhesion of organic coatings.
測試程序旨在評估有機涂層的附著力。
1.1 Purpose
The purpose of this procedure is to determine the resistance to degradation and/or adhesion loss over steel, aluminum, plastic or other substrates coated with organic finishes while subjected to thermal changes and high pressure spray conditions. These conditions are similar to those generated by the heated pressure wash equipment found in manual car wash operations. Evaluation is based on a pass/fail analysis.
本程序的目的是確定在熱變化和高壓噴涂條件下,鋼、鋁、塑料或其他涂有有機涂層的基材的抗降解性和/或附著力損失性。這些情況與手動洗車操作中加熱壓力清洗設備產生的情況相似。評估基于通過/失敗分析。
1.2 Coverage of this Standard
This test procedure may be used to evaluate organic finishes over metal or plastic substrates with
appropriate surface preparation (plating, chemical surface treatment, etc). This test procedure can be used for interior, exterior, and underhood/underbody applications.
本試驗程序可用于評估金屬或塑料基底上的有機飾面,包括 適當的表面處理(電鍍、化學表面處理等)。本測試程序可用于車內、車外和發動機罩下/車身底部應用。
2.0 SPECIAL TEST EQUIPMENT & MATERIALS
試驗設備和材料
TABLE 1: SPECIAL TEST EQUIPMENT | ||
Name Of Item | Description | Make/Model |
Scribe Tool | Straight shank tungsten carbide tipped scribe device with a tip angle of 60 15 degrees or equivalent. | N.A. |
Razor knife | Common utility knife or X-acto knife | N.A. |
Water Bath | Capable of maintaining 38 +/- 2° C with aeration | N.A. |
Freezer | Capable of maintaining -29 +/- 2° C N | N.A. |
Steam Generator 蒸汽發生器 | Discharge Nozzle: 12.5 mm ID (100 mm minimum length) Dynamic Head Pressure: 37.9 +/- 2 kPa (5.5 psi) +/- 5% deviation | Model 100 Steam Generator from Atomic Steam Co., 10727 Fendell, Detroit, MI 48238 or equivalent. |
3.0 SUMMARY OF METHOD
This procedure will evaluate organic coating adhesion after exposure to elevated and reduced
temperatures using high pressure steam impingement.
本程序將評估有機涂層暴露于高溫和低溫環境后的附著力使用高壓蒸汽沖擊的溫度。
4.0 SAFETY PRECAUTIONS
This test procedure involves high and low temperature conditions, steam, and high pressure spray.
Pressurized steam represents a potential burn hazard. Parts must be secured properly to the test fixture and laboratory technicians should wear full face shields and heat resistant gloves. If possible, the testing should be conducted in a test chamber equipped with a full closing front shield with safety interlock to prevent triggering steam with the shield open. This standard does not address all the safety problems associated with its use. It is the responsibility of whomever uses this standard to consult and establish appropriate safety and health practices to determine the applicability of regulatory limitations prior to use.
本試驗程序涉及高溫和低溫條件、蒸汽和高壓噴霧。加壓蒸汽有潛在的燒傷危險。零件必須正確地固定在試驗夾具上,實驗室技術人員應佩戴全面罩和耐熱手套。如有可能,應在配有全封閉前護罩(帶安全聯鎖裝置)的試驗箱中進行試驗,以防止護罩打開時觸發蒸汽。本標準并未解決與其使用相關的所有安全問題。使用本標準的任何人都有責任在使用前咨詢并建立適當的安全和健康實踐,以確定監管限制的適用性。
5.0 CONDITIONING
Condition fully cured parts or panels for a minimum of 72 hours at 23 +/- 2°C and 50 +/- 10% relative humidity prior to beginning test procedure.
在開始試驗程序之前,在23+/-2°C和50+/-10%相對濕度條件下對*固化的零件或面板進行至少72小時的處理。
6.0 PROCEDURE
A. Immerse test specimen in an aerated water bath at 38 2°C for 4 hours. Water should contain max 5 ppm dissolved solids as sodium chloride (NaCl).
將試樣浸入38 2°C的充氣水浴中4小時。水應含有最多5 ppm的溶解固體,如氯化鈉(NaCl)。
B. Immediately after removal from water bath, scribe parts or panels through to the substrate as shown in Figure 1.
從水浴槽中取出后,立即將零件或面板劃入基板,如所示